Cu dispersion in microwave sintered iron compacts


Kusoglu I., Onel K., Willert-Porada M.

European International Powder Metallurgy Congress and Exhibition, Euro PM 2009, Copenhagen, Denmark, 12 - 14 October 2009, vol.3 identifier

  • Publication Type: Conference Paper / Full Text
  • Volume: 3
  • City: Copenhagen
  • Country: Denmark
  • Dokuz Eylül University Affiliated: Yes

Abstract

Gas atomized Cu powder is added to Iron powder in varying amounts and mixed in a V-type mixer for 30 minutes at 15 rpm. As lubricant 1 wt% Acrawax C is used. The mixtures are compacted at 600 MPa to form TRS (Transverse Rupture Strength) samples with dimensions 6,35*12,8*31,8 mm. The samples are sintered using conventional and microwave furnaces for 30 minutes at 1150 °C under 90% N2 -10% H2 atmosphere. The microstructure of sintered specimens and Cu dispersion in Fe are observed by SEM and EDS, and the strength is determined by TRS tests.